| Eigendom | PPA GF30 (Amodel A-1133HS) | PA66 GF30 | PA46 GF30 (Stanyl) | PPS GF40 |
|---|---|---|---|---|
| Dichtheid | 1.47 g/cm³ | 1,36 g/cm³ | 1,41 g/cm³ | 1,65 g/cm³ |
| Smeltpunt | 310–325°C | 260 °C | 295 °C | 280 °C |
| HDT bij 1,80 MPa | 300–310°C | 245–255 °C | 285 °C | 265 °C |
| Trekmodulus (droog) | 12,000 MPa | 9.500–10.500 MPa | 10.000 MPa | 14.000–15.000 MPa |
| Tensile Modulus (conditioned) | ~11,500 MPa | 6,000–7,000 MPa | 6,000 MPa | ~14,000 MPa |
| Tensile Strength (dry) | 200 MPa | 180 MPa | 180 MPa | 190 MPa |
| Tensile Strength (conditioned) | ~180 MPa | 120 MPa | 120 MPa | ~190 MPa |
| Water Absorption (23°C / 50% RH) | 0.3–0.5% | 1.5–2.0% | 2.6% | 0.03% |
| Krimp bij het gieten (in de lengterichting / dwarsrichting) | 0.2% / 0.6% | 0.4% / 1.1% | 0.5% / 1.3% | 0.3% / 0.8% |
| Continuous Use Temp (5000h) | 150–170°C | 120–130 °C | 163 °C | 200–220 °C |
| Relatieve kosten per kg | Hoog | Laag-matig | Matig-Hoog | Hoog |
Key Insight: The Conditioned Modulus Advantage
PPA polyphthalamide materials are chosen for high-heat applications that demand lower moisture absorption than standard nylons.
Look at the “conditioned” tensile modulus row. This is where PPA justifies its price premium.
- PA66 GF30 loses 30–40% of its dry stiffness after moisture conditioning — a known pain point for precision applications in humid environments.
- PA46 GF30 drops even more (40%), because its high amide-group density makes it more hygroscopic than PA66.
- PPA GF30 retains 95%+ of its dry stiffness after conditioning, because the aromatic rings in the backbone block water molecules from hydrogen-bonding with amide groups.
- PPS GF40 is nearly unaffected by moisture, but costs 2–3× PPA.
For structural parts that must hold tight tolerances from dry-as-molded through end-use humidity cycling, PPA’s conditioned modulus advantage is often decisive.


Commercial PPA Grade Selector
| Fabrikant | Merk | Rang | GF % | Belangrijkste kenmerk | Typische toepassing |
|---|---|---|---|---|---|
| Solvay | Amodel | A-1133 HS | 33% | General purpose GF33, heat stabilized | Automotive connectors, housings |
| Solvay | Amodel | AS-1133 HS | 33% | Thick-wall (>3 mm) optimized | Pump housings, valve bodies |
| Solvay | Amodel | A-1145 HS | 45% | High stiffness, heat stabilized | Metal replacement, structural brackets |
| Solvay | Amodel | A-1565 HS | 65% (GF+mineral) | Maximum rigidity, low warpage | Large structural housings |
| Solvay | Amodel | AE-1133 | 33% | Electrical-optimized, high CTI | EV connectors, busbar insulators |
| Solvay | Amodel | A-4122 NL WH | 22% | LED reflectors, high whiteness | Automotive lighting, LED chips |
| DuPont | Zytel HTN | 51G35HSL | 35% | Standard GF35, heat stabilized | Engine covers, oil pans |
| DuPont | Zytel HTN | 51G45HSL | 45% | High stiffness PA6T-based | Structural underhood parts |
| DuPont | Zytel HTN | 52G35HSL | 35% | 6T/66 copolymer, better flow | Thin-wall connectors |
| DuPont | Zytel HTN | 54G15HSLR | 15% | Low GF, high ductility | Snap-fit clips, flexible mounts |
| Kuraray | Genestar | GP2300 | 30% | PA9T GF30, lowest moisture | SMT connectors, precision electronics |
| Kuraray | Genestar | GR2300 | 30% | PA9T GF30 FR V-0 | USB connectors, mobile device internals |
| EMS | Grivory | GV-5H | 50% | High-strength PA6T/6I | Metal replacement, structural |

PPA Processing Guidelines
| Parameter | Aanbevolen waarde | Opmerkingen |
|---|---|---|
| Voordrogen | 120°C for 4 hours | Desiccant dryer. Target moisture < 0.05% |
| Smelttemperatuur | 320–340 °C | Varies by grade; PA6T grades need 330°C minimum |
| Schimmel Temperatuur | 120–160°C | Higher than PA66 — oil-heated molds typically required |
| Injectiesnelheid | Gemiddeld tot snel | Fast fill to avoid premature skin formation |
| Druk vasthouden | 60–100 MPa | PPA has low shrinkage; pack adequately |
| Verblijftijd | Minimaliseren (≤ 5 min) | Degradation risk increases above 330°C |
Belangrijke opmerkingen over de verwerking:
- Mold temperature is non-negotiable: PPA requires mold temperatures of 120–160°C to achieve full crystallinity. Running at standard nylon mold temperatures (80°C) produces amorphous, dimensionally unstable parts. Oil-heated or electric cartridge-heated tooling is typically necessary — water-heated molds won’t reach these temperatures.
- High barrel temperature management: At 330°C, standard nylon purging procedures apply, but residence time must be tightly controlled. PPA degradation produces volatiles; verify adequate mold venting.
- Low and predictable shrinkage: PPA’s shrinkage (0.2% flow direction for GF grades) is lower than both PA66 and PA46. This is an advantage for precision, but molds designed for PA66 may need gate and runner adjustments when switching to PPA.
- Fast crystallization once below Tm: Unlike PA46 (which crystallizes fast at all temperatures), PPA crystallizes rapidly once the melt drops below its melting point — but reaching that point requires the mold to be hot enough. This is the fundamental trade-off of PPA processing: high mold temp for crystallization vs. cycle time.
Key PPA Applications by Industry
| Industrie | Toepassing | Why PPA Over PA66 or PA46 |
|---|---|---|
| Automotor | Coolant pump housings, thermostat housings, oil filter bodies | Glycol resistance + dimensional stability at 120–150°C |
| Automotive Fuel | Fuel line connectors, quick-connects, sender unit bodies | Fuel resistance, low permeation, survives aggressive blended fuels |
| Automotive Transmission | Solenoid bobbins, sensor housings | Hot ATF resistance, stable dielectric properties |
| Elektriciteit / Elektronica | SMT connectors, USB-C housings, DDR sockets, SIM card trays | Survives 260°C reflow, retains dimensions, UL94 V-0 grades available |
| Vermogenselektronica | Busbar insulators, IGBT housings, EV charging connector bodies | High CTI (Comparative Tracking Index), arc resistance |
| Consumentenelektronica | Mobile device frames, smartwatch housings, laptop chassis inserts | Thin-wall flow, paintable, dimensionally stable across humidity range |
| Industrieel | Pump wear rings, bearing cages, valve seats | Creep resistance + chemical compatibility |
PPA vs. PA46: Choosing Between the Two
PPA and PA46 are often cross-shopped for the same applications. Here is the decision framework in practice:
| Selection Driver | Choose PPA When | Choose PA46 When |
|---|---|---|
| Moisture / humidity exposure | High humidity, outdoor, or condensing environments | Controlled indoor environments |
| Blootstelling aan chemische stoffen | Fuel, glycol, aggressive automotive fluids | Primarily oil, grease, or dry applications |
| Cyclustijd | Longer cycles acceptable (mold 140°C) | Need fastest cycle times (mold 100°C works) |
| Thin-wall flow | Good (walls down to 0.4 mm) | Excellent (walls down to 0.2 mm) |
| Wear / friction | Good with internal lubricants | Excellent — PA46 is the benchmark |
| Dimensional tolerance in wet/dry cycling | PPA wins — almost no change from dry to conditioned | Expect 0.2–0.5% dimensional change |
| Gereedschapskosten | Higher (oil-heated mold required) | Moderate (water-heated mold usually sufficient) |
| Price / kg | Hoger | Matig |

PPA Limitations: When to Look Elsewhere
- Investeringen in gereedschap: PPA’s 120–160°C mold temperature requirement means water-heated molds cannot be used. If your tool shop is not equipped for oil or electric mold heating, you will incur tooling modification or replacement costs.
- Gevoeligheid van de inkeping: Standard GF PPA grades are notch-sensitive — impact in notched sections is lower than you might expect from the tensile data. For snap-fit parts requiring toughness, specify impact-modified grades (e.g., Zytel HTN 54G series).
- Above 180°C continuous: PPA’s continuous use ceiling is 150–170°C (UL RTI). For sustained exposure above 180°C you need PPS or PEEK.
- Cost-sensitive projects: PPA GF30 costs 3–5× PA66 GF30. Make sure you actually need the performance before specifying it.
What Is PPA?
PPA (polyphthalamide) is a family of semi-aromatic polyamides. Unlike standard aliphatic nylons like PA6 and PA66 — whose polymer backbones are built entirely from aliphatic carbon chains — PPA incorporates aromatic rings (terephthalic or isophthalic acid) directly into the polymer backbone. This structural difference is what gives PPA its defining advantage: dramatically lower moisture absorption, better dimensional stability in humid environments, and 20–40% higher strength retention at temperature compared to PA66.
The PPA family is not a single polymer but a class of high-performance nylons defined by the aromatic diacid used. The main commercial variants are PA6T, PA9T, PA10T, and various copolymers sold under brand names including Solvay Amodel, DuPont Zytel HTN, Kuraray Genestar, and EMS Grivory.
Voor ingenieurs en inkopers die op zoek zijn naar PPA datasheets, PA6T vs PA9T comparison, or PPA vs PA66 vs PA46 selection guidance, this page consolidates the key properties, grade families, processing parameters, and application data.
PPA Sub-Families: PA6T, PA9T, PA10T — What’s the Difference?
| Variant | Base Diol | Tm (°C) | Belangrijkste voordeel | Typical Brands | Limitation |
|---|---|---|---|---|---|
| PA6T | Hexamethylene diamine (C6) | 310–325 | Highest HDT, broadest grade portfolio | Amodel (Solvay), Zytel HTN 51G (DuPont) | Pure PA6T Tm exceeds decomposition temp; always copolymerized |
| PA9T | Nonamethylene diamine (C9) | 306–315 | Lowest moisture absorption, excellent solder resistance | Genestar (Kuraray) | Higher cost, fewer FR grades |
| PA10T | Decamethylene diamine (C10) | 290–310 | Bio-based (castor oil derived), good flow | Vestamid HTplus (Evonik), Grivory (EMS) | Lower HDT than 6T, newer product |
| PA6T/66 | C6 + adipic acid | 290–310 | Improved flow, lower cost | Zytel HTN 52G, 54G (DuPont) | Higher moisture absorption than pure 6T |
| PA6T/6I | C6 + isophthalic acid | Amorf | Transparency, barrier properties | Selar PA (DuPont) | Not for structural applications |
PPA GF30 vs. Competing High-Temperature Materials

PPA Engineering Notes
PPA and PA66 Material Boundary
PPA (polyphthalamide) is a semi-aromatic polyamide, while PA66 is a fully aliphatic polyamide. PPA incorporates aromatic acid groups (terephthalic/isophthalic acid) into its polymer backbone, which reduces moisture absorption from ~2% (PA66) to ~0.3–0.5% (PPA). This means PPA retains its mechanical properties in humid environments, withstands 30–50°C higher continuous-use temperatures, and resists chemical attack from fuels and glycols better than PA66. The trade-off is higher cost and more demanding processing requirements.
PPA Family and PA6T Grades
PA6T is the most common sub-type of PPA, but not the only one. PPA is the family name; PA6T, PA9T, PA10T, and various copolymers (PA6T/66, PA6T/6I) are specific members. PA6T-based grades (Amodel, Zytel HTN 51G) dominate the automotive and industrial markets. PA9T (Genestar) has carved a niche in consumer electronics due to its even lower moisture absorption. Always check which base chemistry is used in a PPA grade — it affects moisture uptake, processing window, and cost.
PPA Drying Before Molding
Yes — and with tighter requirements than PA66. PPA must be dried to below 0.05% moisture content (PA66 allows up to 0.20%). At PPA’s 330°C processing temperature, any residual moisture causes hydrolysis that degrades molecular weight and produces visibly defective parts. Dry at 120°C for a minimum of 4 hours in a desiccant dryer.
PPA for SMT Components
Yes — this is one of PPA’s core markets. Standard PPA GF30 grades (especially PA9T Genestar) survive lead-free reflow soldering with peak temperatures of 260°C without blistering or warping. This is why PPA dominates SMT connector housings (USB, HDMI, DDR memory sockets, SIM card trays) where the plastic must survive the solder reflow oven and then maintain precise contact spacing in end-use humid environments.
PPA Tradeoffs Compared with PA46
PPA processes slower (higher mold temperature required), costs more per kilogram, and is typically more notch-sensitive than PA46. PA46 cycles faster and flows better in very thin walls (< 0.3 mm). However, PPA's conditioned modulus advantage and chemical resistance often outweigh these processing trade-offs in demanding applications.
Need PPA pellets, technical datasheets, or grade selection support? We supply Amodel, Zytel HTN, and Genestar grades in GF10 to GF50 reinforcement levels. Contact us with your temperature, chemical exposure, and production volume requirements.
Veelgestelde vragen
Bekijk onze PA66 GF33 vs GF40 vs GF60 comparison voor gedetailleerde informatie over de selectie van woningklassen en woninggegevens.
What is the difference between PPA and standard nylon?
PPA (polyphthalamide) incorporates aromatic groups in the polymer backbone, giving it significantly higher glass transition temperature (120-140°C vs. 50-60°C for PA66), better chemical resistance, and much lower moisture absorption. PPAs bridge the gap between standard nylons and high-cost specialty polymers like PEEK.
Which PPA grade is best for automotive under-hood applications?
PA6T/66 and PA6T/6I copolymers are preferred for under-hood parts requiring continuous use at 150-180°C. Grades like Solvay Amodel and BASF Ultramid Advanced N offer excellent coolant and oil resistance, making them suitable for thermostat housings, water pump components, and charge air cooler end caps.
How does PPA PA9T differ from PA6T?
PA9T (polyphthalamide 9T) uses a longer C9 diamine (nonanediamine), giving it lower moisture absorption than PA6T. It processes at slightly lower temperatures and offers better flow characteristics, making it suitable for thin-wall electrical connectors. PA6T generally has higher heat resistance.
What are bio-based PPAs like PA10T?
PA10T uses sebacic acid derived from castor oil as one monomer, making it partially bio-based (40-60% renewable content). PA10T offers excellent chemical resistance and low moisture absorption similar to PA12, but with better heat resistance. It is increasingly specified in automotive fuel system and cooling circuit components.
How should a buyer compare PPA vs PA66 for a high-temperature part?
Compare actual reinforced or modified grades against the same continuous and peak temperature, load duration, humidity, fluid exposure and dimensional limits. Melting point alone does not establish service life. Include the incumbent grade and failure mode in a replacement request, and agree the conditioning, heat-aging or fluid tests that will approve the candidate before comparing the material and tooling quotations.
Last updated: June 2026. Datasheet values are typical ranges. Always verify specific grade properties with the manufacturer’s current technical data sheet. Amodel is a registered trademark of Solvay. Zytel HTN is a registered trademark of DuPont. Genestar is a registered trademark of Kuraray. Grivory is a registered trademark of EMS-Chemie.
Gerelateerde lezen
- Stanyl PA46-gids: Eigenschappen van Nylon 46 GF30 en GF40 bij hoge temperaturen vergeleken met PA66 en PPA
- Gids voor LCP (vloeibaar-kristallijn polymeer): Type I, II en III, eigenschappen van Vectra en Zenite, en LCP versus PPS versus PEEK
- Polycarbonaat (PC) — Volledige gids over technische eigenschappen en industriële toepassingen